Laticpave 丙烯酸弹性涂料
Acrylic Cushion Coatings
 
   
  • 彩色面料
    Color Coatings
  • 丙烯酸弹性胶浆
    Cushion Coatings
  • 新水泥基础底漆
    Primer for Concrete
  • 基础修补料
    Patching Mortar

 

1、LATICPAVE 彩色涂料的配制是按以下比例加入60-120目石英沙作为纹理层用料:彩色面涂:石英沙:水=15加仑:50-75kg:12-15加仑按上述顺序边加边搅,直至搅匀。
2、配置好的料用1米的胶耙刮到场地上。约2小时表干,气温低时需更长的时间。 
3、面涂层不用或少加石英沙,配料比例 彩色面涂:石英沙:水=15加仑:50-75kg:12-15加仑 按上述顺序边加边搅拌,直至搅匀.气温低时需更长的时间。
注意事项
1 不要在一小时内会下雨时施工
2 水泥基础处理请咨询本公司技术部门
3 如果用于软垫弹性面层,应购买本公司适应弹性基础的彩色面涂
包装
55加仑 or 5加仑
储存
避免阳光暴晒和底于0 C以下温度储存储存期一般为半年

LATICPAVE Color Coatings produced by IPN technology of which composed of two special functional bases in molecule chains ;Therefore qualities from advantages of two resins such as adhesives, waterproofness,resistance corrosion etc,are perfectly composed with together.
Usage
Mix as texture layer with 60-120mesh silicone sand according to ratio below:Color coating:silicone sand:portable water=15cal:50-75kg:15cal Add materials in sequence above
As finish layer there is not any sand or few to add in when mix it.
Apply the mixage with 1 metre squilgee on base,Surface dry needs 2 hours.
Warranty
1 Do not apply them when it showering in an hour.
2 When it applied on concrete base,please enqury on technical department of supplier with no hesitate.
3 When it will be applied as finishing or texture of cushion coatings,you'd better inform to supplier
Package
55cal or 5cal
Shelf
Avoiding under sunshine in direct or store below 0C tempareture
Shelflife is a year

 

良好的弹性,增加了运动的舒适性;富裕起来的国情开始使人们不再满足硬 地简易球场的感觉,越来越多的球场开始使用软垫弹性丙烯酸材料。通过科 学的工艺,使本公司软垫丙烯酸材料成为造价最低,但质量上乘的弹性丙烯 酸球场材料;再加上本公司处理水泥基础的成熟可靠的技术,本公司和使用 本公司产品的客户用之翻新改造了大量球场,获得了可观经济和社会效益。

LATICPAVE超级软垫涂层施工方法
1.基础处理 
水泥基础场地先进行包括酸洗,打底胶,修补等必要的处理。可根据水泥基 础场地实际情况向本公司咨询实际处理方案;沥青基础场地则无需上述基础 处理。 
2.施工弹性缓冲层
a.配料:先将弹性胶料3×5加仑倒入55加仑大铁桶,加入一包(40公斤) 黑胶粒,一边加水,一边搅拌,总加水量为(3至4)×5加仑,具体加水量可 根据掌耙师的要求加,一定不要一次加完。然后再加半包或一包黑胶粒搅匀。
b.施工方法:如一般施工彩色丙烯酸涂料一样施工,即用胶耙现场刮耙。 一个场地每一道要用上述配料方法配制的三大桶料,即3×55加仑配好的料。
3.封顶层施工 
弹性缓冲层施工完后,表面不会完全平整密实,需用弹性胶浆加细胶粉和石 英砂封填平整。方法如同上述配黑胶粒一样。施工方法也一样。
4. 施工彩色面层
缓冲层达到基本平整后,即可施工彩色涂层。包括加砂纹理层两道,无沙面 层一至两道。方法如一般硬地丙烯酸球场施工。只是此处的彩色面层应有一 定的弹性,能承受一定的强力冲击而不会龟裂。   
5. 划线。
注意事项
1.温度低于10摄氏度时不宜施工丙烯酸涂料。
2.将要下雨时,也不要急于施工。
3.材料不要放在太阳下暴晒,也不可储存在会结冰的地方.
Method of Application
1 Prepare of Base
The procedure such as acid corrosion ,priming and resurfacing should not be  omitted for cememt concrete base than that of asphalt concrete.
2 Construction of Cushion
Mix: pour 3 pails 5 cal coat into a 55cal barrel,add 40kg SBS granules with water adding then mixing them .Total of water is no more than 20 cal for a barrel mixing.
At last another 20kg granule is added into,mixs  homogenousely . It is as same  as the application of the color coatings
3 Top Coating Construction
The coating of cushion is not more smooth. The mix of SBS powder with glues should be applied at least once to twice to resurface the surface of cusion. 
4 Application of Color Coatings
Color coatings should be including the two applications of texture coatings and  at least one application of finishing coating 
5 Lining.
Limitations and Precautions
Should not be applied when ambient temperature is below 50 F or when the surface temperature is above 140F.Do not apply when rain is imminent.Do not store in direct sunlight.Keep from freezing.  

 

球场基础有时候很差,有比较厚的积水或低洼处需找平,超过一定的厚度往往需要分多次补平。采用修补砂浆则不需要面临这个问题了。使用修补砂浆,可以一次不很厚也不开裂,并且能快速干透,不会带来后患。
使用方法
根据实际需要取修补砂浆一份,加入0.2-0.3份配给的修补料,加水不超过0.2份水,混合均匀即可,切忌加太多水引起开裂,修补厚度达不到。
Bird water often ocurs on substrate,it is trouble that resurfacing many times need for too thickness.The material solves the trouble but no crack ocurs and cure rapidly.
Application
I part mortar mixes with 0.2-0.3 resufacing coating and 0.2 part water.Do not add water than specified.

 

球场基础有时候很差,有比较厚的积水或低洼处需找平,超过一定的厚度往往需要分多次补平。采用修补砂浆则不需要面临这个问题了。使用修补砂浆,可以一次不很厚也不开裂,并且能快速干透,不会带来后患。
使用方法
根据实际需要取修补砂浆一份,加入0.2-0.3份配给的修补料,加水不超过0.2份水,混合均匀即可,切忌加太多水引起开裂,修补厚度达不到。
Bird water often ocurs on substrate,it is trouble that resurfacing many times need for too thickness.The material solves the trouble but no crack ocurs and cure rapidly.
Application
I part mortar mixes with 0.2-0.3 resufacing coating and 0.2 part water.Do not add water than specified.

 
 
 