Laticpave 硬地丙烯酸涂料
Acrylic Hard Coatings
 
   
  • 彩色面料
    Color Coatings
  • 丙烯酸底涂
    Acrylic Resurfacer
  • 新水泥基础底漆
    Primer for Concrete
  • 基础修补料
    Patching Mortar

 

1、LATICPAVE 彩色涂料的配制是按以下比例加入60-120目石英沙作为纹理层用料:彩色面涂:石英沙:水=15加仑:50-75kg:12-15加仑按上述顺序边加边搅,直至搅匀。
2、配置好的料用1米的胶耙刮到场地上。约2小时表干,气温低时需更长的时间。 
3、面涂层不用或少加石英沙,配料比例 彩色面涂:石英沙:水=15加仑:50-75kg:12-15加仑 按上述顺序边加边搅拌,直至搅匀.气温低时需更长的时间。
注意事项
1 不要在一小时内会下雨时施工
2 水泥基础处理请咨询本公司技术部门
3 如果用于软垫弹性面层,应购买本公司适应弹性基础的彩色面涂
包装
55加仑 or 5加仑
储存
避免阳光暴晒和底于0 C以下温度储存储存期一般为半年

LATICPAVE Color Coatings produced by IPN technology of which composed of two special functional bases in molecule chains ;Therefore qualities from advantages of two resins such as adhesives, waterproofness,resistance corrosion etc,are perfectly composed with together.
Usage
Mix as texture layer with 60-120mesh silicone sand according to ratio below:Color coating:silicone sand:portable water=15cal:50-75kg:15cal Add materials in sequence above
As finish layer there is not any sand or few to add in when mix it.
Apply the mixage with 1 metre squilgee on base,Surface dry needs 2 hours.
Warranty
1 Do not apply them when it showering in an hour.
2 When it applied on concrete base,please enqury on technical department of supplier with no hesitate.
3 When it will be applied as finishing or texture of cushion coatings,you'd better inform to supplier
Package
55cal or 5cal
Shelf
Avoiding under sunshine in direct or store below 0C tempareture
Shelflife is a year

 

水泥基础球场最好使用丙烯酸底涂。LATICPAVE底涂采用先进的技术合成的树脂;其含有特殊官能基能后交联成膜。此性质赋予了LATICPAVE底涂机械稳定性,因而在水泥基础上仍有很好的粘结性;因此该底涂尤其适合解决水泥基础上涂层起泡脱落的问题。. 
使用方法
1、LATICPAVE底涂的配制是按以下比例加入到少325标号水泥和60-120目石英沙:底涂:石英沙:水泥:水=15加仑:50-75kg:25kg:15加仑 按上述顺序边加边搅,直至搅匀。
2、配置好的底料用1米的胶耙刮到场地上。约2小时表干,气温低时需更长的时间。  

LATICPAVE Resurfacer is synthesized with the advanced technology of latex,composed of special functional base in molecule chain against the alkali corrosion from the cement.Therefore the cured coat is not easily damaged by the newly-cured concrete
Usage
Mix it with 60-120mesh silicone sand and 325# portland cement according to ratio below: Resurfacer:siliconesand:cement:portable water=15cal:50-75kg:25kg:15cal Add materials with sequence aboveApply the mixage with 1metre squilgee on base,Surface dry needs 2 hours.  
Warranty
1 Do not apply them when it showereing in an hour.
2 When it applied on concrete base, please enquiry to technical department of supplier with no hesitance.
3 When it will be applied as finishing or texture of cushion court, you'd better inform to supplier

Package           55gal or 5gal

Shelf
Avoiding shelf under sunshine in direct or store below 0oC tempareture
Shelflife is a year

 

 

 

球场基础有时候很差,有比较厚的积水或低洼处需找平,超过一定的厚度往往需要分多次补平。采用修补砂浆则不需要面临这个问题了。使用修补砂浆,可以一次不很厚也不开裂,并且能快速干透,不会带来后患。
使用方法
根据实际需要取修补砂浆一份,加入0.2-0.3份配给的修补料,加水不超过0.2份水,混合均匀即可,切忌加太多水引起开裂,修补厚度达不到。
Bird water often ocurs on substrate,it is trouble that resurfacing many times need for too thickness.The material solves the trouble but no crack ocurs and cure rapidly.
Application
I part mortar mixes with 0.2-0.3 resufacing coating and 0.2 part water.Do not add water than specified.

 

球场基础有时候很差,有比较厚的积水或低洼处需找平,超过一定的厚度往往需要分多次补平。采用修补砂浆则不需要面临这个问题了。使用修补砂浆,可以一次不很厚也不开裂,并且能快速干透,不会带来后患。
使用方法
根据实际需要取修补砂浆一份,加入0.2-0.3份配给的修补料,加水不超过0.2份水,混合均匀即可,切忌加太多水引起开裂,修补厚度达不到。
Bird water often ocurs on substrate,it is trouble that resurfacing many times need for too thickness.The material solves the trouble but no crack ocurs and cure rapidly.
Application
I part mortar mixes with 0.2-0.3 resufacing coating and 0.2 part water.Do not add water than specified.

 
 
 

广州金力美建材实业有限公司
工信部备案/许可证号:粤ICP备17021946号
版权所有,抄袭必究
Tel:020-82581086 Fax:020-82037502